26
A
-en
English
⋅
Fornax
®
T
en
Casting table
Alloys
Continuous
heating /
holding time*
Preheating temperatures
Crucible
and
insert
Melting
powder
Au
LFC
BioPlatinLloyd
®
14...17 sec
700 °C
(1290 °F)
-- Auromelt
✔
BioPontoStar
®
15...18 sec
850 °C (1530 °F)
✔
BioPontoStar
®
XL
17...22 sec
850 °C (1530 °F)
LFC
PlatinLloyd
®
KF
10...13 sec
700 - 750 °C (1290 - 1380 °F)
-
PlatinLloyd
®
M/100
10...13 sec
700 °C (1290 °F)
✔
PontoLloyd
®
G
22...25 sec
850 °C (1530 °F)
✔
PontoLloyd
®
P
18...22 sec
850 °C (1530 °F)
LFC
Pontonorm
12...15 sec
700 °C (1290 °F)
✔
PontoStar
®
G/H
17...20 sec
850 °C (1530 °F)
Au
LFC
AuroLloyd
®
KF
17...20 sec
700 °C (1290 °F)
-
AuroLloyd
®
M
17...20 sec
700 °C (1290 °F)
✔
BegoCer
®
G
12...18 sec
850 - 950 °C (1530 - 1740 °F)
-- Auromelt
✔
BegoStar
®
22...25 sec
850 °C
(1530 °F)
Pd
✔
BegoPal
®
/S
13...16 sec
850 °C (1530 °F)
-- Auromelt
✔
BegoPal
®
300
13...16 sec
850 - 950 °C (1530 - 1740 °F)
-- Auromelt
Ag
LFC
BegoStar
®
LFC
17...20 sec
700 °C (1290 °F)
-- Auromelt
LFC
ECO d’OR
17...20 sec
700 °C (1290 °F)
Eco
✔
BegoStar
®
ECO
07...11 sec
850 °C (1530 °F)
-- Auromelt
NiCr
✔
Wirocer plus
06...12 sec
900 - 950 °C (1650 - 1740 °F)
✔
Wiron
®
99
07...10 sec
900 - 950 °C (1650 - 1740 °F)
✔
Wiron
®
light
03...07 sec
800 °C (1472 °F)
CoCr
✔
Wirobond
®
C
07...10 sec
900 - 1000 °C (1650 - 1830 °F)
LFC
Wirobond
®
LFC
04...08 sec
900 - 1000 °C (1650 - 1830 °F)
✔
Wirobond
®
SG/280
02...04 sec
900 - 1000 °C (1650 - 1830 °F)
-
Wironit
®
07...10 sec
950 - 1050 °C (1740 - 1920 °F)
-
Wironit
®
LA
06...08 sec
950 - 1050 °C (1740 - 1920 °F)
Wironit
®
extra-hard
02...10 sec
950 - 1050 °C (1740 - 1920 °F)
-
WIRONIUM
®
02...04 sec
950 - 1050 °C (1740 - 1920 °F)
-
WIRONIUM
®
extra-
hard
06...08 sec
950 - 1050 °C (1740 - 1920 °F)
-
WIRONIUM
®
plus
06...08 sec
950 - 1050 °C (1740 - 1920 °F)
* The determined continuous heating times correspond with our technical process experience with castings using
exclusively new materials and are provided as recommendations. The specified values may deviate depending on
the specific alloys, in particular when using non-BEGO alloys.
Note: The table on the following page is provided to record individually determined continuous heating times.
** A glassy-carbon insert may be used as an alternative to the ceramic insert.
**
**