OM-498 Page 47
Return To Table Of Contents
12-19. Troubleshooting − Burn-Through
Burn-Through − weld metal melting completely through base metal resulting
in holes where no metal remains.
Possible Causes
Corrective Actions
Excessive heat input.
Select lower amperage. Use smaller electrode.
Increase and/or maintain steady travel speed.
12-20. Troubleshooting − Waviness Of Bead
Waviness Of Bead − weld metal that is not parallel and does not cover
joint formed by base metal.
Possible Causes
Corrective Actions
Unsteady hand.
Use two hands. Practice technique.
12-21. Troubleshooting − Distortion
Distortion − contraction of weld met-
al during welding that forces base
metal to move.
Base metal moves
in the direction of
the weld bead.
Possible Causes
Corrective Actions
Excessive heat input.
Use restraint (clamp) to hold base metal in position.
Make tack welds along joint before starting welding operation.
Select lower amperage for electrode.
Increase travel speed.
Weld in small segments and allow cooling between welds.