3
Heating Cable Repair
50
|
nVent.com
Apply a small amount of flux to the twisted conductors.
Avoid contaminating the magnesium oxide at the face of
the cable with flux as this will lead to failure during testing.
Heat conductors with the oxy-acetylene torch (this does
not take much heat) and at the same time, touch the
brazing rod to the end of the twisted conductors and
apply enough braze to form a small bead (Figure 64).
Brazing rod
Figure 64: braze twisted conductors
Slightly fan torch back and forth several times to draw
the silver braze backwards, about 1/4 in (6 mm), along
the twisted conductors. Remove heat.
Care must be taken to avoid over-heating the conductors
and to avoid depositing an excessive amount of braze on
the twisted conductors.