30
3DISON PRO
User Manual V.1
3DSION Metal Clay Printing
2) Copper/Bronze/Steel paste
①
Take out output clay with the tile and dry it for 24 hours by natural drying or dry it by
warming for at least 1 hour using a dryer. Print-out has been completely dried can be de-
tached from the tile easily.
②
Prepare firing for dried sample using cube and carbon which are optional items. Build
up about 3cm of carbon on the cube and put the sample on it and bury the sample entirely
by pouring carbon on the sample as much as possible and then close the cover.
<Comparison of set temperature and firing time by material>
Copper
Bronze
Steel
③ Upon completion of firing, switch off the kiln and open the door to cool down the heat
enough. If the heat cools down to room temperature, finish work by taking the sample out
of the cube and brushing the sample using stainless steel brush.
NOTE : Cube and carbon are recyclable (only the part which has not changed into white ash
by oxidation).
※
TIP
Be careful of scald when use toast oven or kiln and especially, in case the output has been
fired in kiln, cool the output enough by opening the door at least an hour before take the printed
object out of the kiln.
When you print in the tile after dry in toast oven, the output will not be separated easily unless
you cool it enough so cool it for at least 30 minutes before you separate the output and then put
it on wire mesh and put in the kiln.
Set temperature: 980°C
Firing time: 4 hours total
Set temperature:
130°C>>843°C
Firing time: 9 hours total
*
After set at 130°C,
increase by 130°C per an
hour up to 843°C. I.E.
130°C>260°C>390°
C>520°C>650°C>780°C>843°C
Set temperature:
778°>>990°C
Firing time: 1 hour in 778°C,
additional firing in 990°C for
2 hours
Annex1. Exchanging the Extruder for the Metal Clay Printing